Laser & CNC
They Cut Stone on a Desktop CNC. Then They Put the Part in a Kiln.
Two makers documented a small CNC and kiln experiment, including visible cracks and the measurements that matter.

The grey part and the reddish one in these photographs started as the same sort of material. The change wasn't a coat of paint. It came after the makers machined soapstone and fired a sample at high temperature.
Michael Perrone and River Burgess documented the experiment as Machining Ceramics on CNC Routers. Their question was whether a relatively soft stone could be shaped on a small CNC and then transformed by firing into a harder material.
It's a fascinating crossover between machining and ceramics—and the photos don't pretend everything went perfectly. One early part wasn't usable and was repurposed for a firing experiment. There is visible cracking in the documented result. That makes it a much better story than a tidy “just press start” headline.
The work was posted in 2023. We haven't repeated the experiment, measured the material or tested the resulting parts. This is a look at what the creators documented, what remains uncertain and why the process is not a casual home-CNC recipe.
First comes the soft-looking part

The team's machined sample before firing. Photo: Michael Perrone and River Burgess / Hackaday.io, CC BY 4.0; resized.
Soapstone can be soft enough to carve, but it isn't one perfectly consistent material. The team notes that its properties vary with mineral content. That means a source, grade and sample matter: “soapstone” on a label isn't enough information to predict how a different piece will behave.
The makers used a desktop CNC to cut a small shaped part. In the photograph, the tool marks are visible across the surface. Those steps and curves are the kind of detail you might associate with a machined plastic or wooden prototype, but here they're in stone.
The goal wasn't merely to make a decorative grey block. The team was exploring whether the material could be shaped first and then heat-treated for applications where a harder ceramic-like result might be useful.
The machine made more than the shape

The documented machining process. The visible dust is a hazard, not a recommended setup. Photo: Michael Perrone and River Burgess / Hackaday.io, CC BY 4.0; resized.
The photographs show a lot of fine dust around the work. The makers used a plastic enclosure in their initial test but explicitly reported that there was still considerable exposure and discussed investigating other controls.
That's an important distinction. A box that keeps your bench looking cleaner does not establish that airborne dust is controlled. Stone composition varies, and cutting or grinding materials containing crystalline silica can generate hazardous respirable dust. NIOSH's silica guidance discusses controls such as appropriate wet methods and local exhaust ventilation.
If you don't know the composition of a stone or have suitable equipment, extraction and procedures, don't machine it. Check the material's safety information and local requirements with a qualified source. This article is about a documented experiment, not an instruction to put an unknown rock under your laser or CNC.
The first sample wasn't a perfect success
The team reports that its first full part needed adjustments during machining and wasn't usable as the intended part. Rather than hide it, they used it to explore the firing process.
I love this kind of documentation. A failed component can still answer a useful question. In this case, it gave the makers something real to measure and compare after heat treatment.
That doesn't mean deliberately wasting material is a great strategy. It means deciding what you can learn from a part that has already gone wrong. Can it become a fit test, a finish sample, a material coupon or a photograph that explains the next version?
Then the colour changed—and a crack appeared

The fired sample in the team's before-and-after comparison. Photo: Michael Perrone and River Burgess / Hackaday.io, CC BY 4.0; resized.
After firing, the pictured sample is visibly different in colour. The documentation also shows a crack in a later fired part and discusses possible warping. This is the bit that prevents me from calling it a neat shortcut to a production-ready ceramic part.
The project's initial measurements reported changes from 60.95 to 61.7 mm in length, 40.35 to 40.64 mm in width and 23.09 to 23.07 mm in height for one sample. Those are the creators' figures for their experiment, not general shrinkage values you can safely apply to another piece of stone.
Even a small dimensional change can matter if a part has to fit a bearing, mate with a fastener or sit flat against another surface. A pretty colour change is interesting. A measured fit after firing is what would answer the practical question.
About that kiln
The creators discuss firing in the region of 1,000–1,200 °C. That requires suitable high-temperature equipment and expertise; it's not a normal kitchen-oven experiment. Heating unknown stone can also introduce hazards and unpredictable failure.
We're not providing a firing schedule here or suggesting readers copy the setup. Anyone considering stone machining or kiln work needs the correct material information, controls and experienced guidance for the specific process. Treat the project as an exploratory case study, not a tested safety procedure.
The researchers suggest possible uses such as heat-resistant parts and moulds, while also acknowledging variability and warping. Those are potential directions, not proven suitability for a specific high-temperature, electrical or structural application.
What the experiment teaches a CNC maker
You don't need to work with soapstone to take something from this. The team's sequence exposes several familiar workshop questions:
- What exactly is the material? Two pieces with the same broad name can behave differently.
- What changes after machining? Heat, moisture, finish or adhesive can alter a part that initially fitted.
- What should be measured? Pick the dimensions and properties that matter to the final job, not just the ones that are convenient.
- What did the failed part reveal? A documented crack or awkward cut can guide the next test.
- Are the controls adequate? A photograph of a setup isn't proof that the dust or heat risks are managed.
You can apply those questions to wood that moves after finishing, an acrylic assembly with a tight fit, or a 3D print that distorts after sitting in a hot car. Different materials, same need to test the real conditions.
A better way to look at a dramatic result

A crack in a later fired sample. Photo: Michael Perrone and River Burgess / Hackaday.io, CC BY 4.0; resized.
The striking part of the project isn't that a desktop machine magically became a ceramics factory. It's that the makers asked a precise question, documented a first attempt and showed enough of the imperfect result for someone else to learn from it.
You can read the project and initial test log for the original photographs and measurements. The creators mark the work CC BY 4.0; credit them and check the terms of any separately supplied material before reuse.
For me, the useful takeaway is simple: a part isn't finished just because it came off the machine. Sometimes the really interesting test happens afterwards.
Sources
Share this article
Know someone who would enjoy this? Pass it along.